MA625

Ni-21.5Cr-9Mo-2.5Fe-3.7Cb+Ta(mass%)
Nickel chrome alloy featuring outstanding aspects both in corrosion resistance and heat resistance.

Aerospace & Energy Materials Dept.

Main Features

This alloy has particularly excellent corrosion and oxidation resistance. It shows high level of strength, rupture strength and fatigue strength qualities at wide specter of temperatures - from very low up 1100°C.
MA625 is a nonmagnetic alloy. It is a Ni-Cr type alloy with Mo and Cb added to improve strength and corrosion resistance. It especially shows successful results in stress corrosion cracking sensitivity induced by chloride ions. It is mainly used for Jet engine parts, aircraft materials, chemical industry parts, special sea water equipment, heat furnace material, evaporators.

Weldability/Workability

MA625 is not suitable for oxy-acetylene method. However, other welding methods are applicable and it has weldability close to that of 18Cr-8Ni Stainless steel. Welding congelation cracking sensitivity is lower than the 25Cr-20Ni Stainless steel type alloys, and only a little higher than the MA-X alloys.

Available Product Forms

Various shapes, such as flat-rolled plates, forgings, welding wires, wires, welded pipes and tubes, seamless pipes and tubes can be manufactured.

Specifications

Information on specifications to which MA625 alloy can be ordered.

ASTM UNS N06625

Plates Bars, Forgings Pipes and Tubes Joints
B443 B446 B444 B366
  B564 B704  
    B705  

ASME UNS N06625

Plates Bars, Forgings Pipes and Tubes Joints
SB-443 SB-446 SB-444 SB-366
  SB-564 SB-704  
    SB-705  

JIS NCF625

Plates Bars Pipes and Tubes
G4902 G4901 G4903
    G4904

AMS UNS N06625

Plates Bars Pipes and Tubes
5599 5666 5581

Mechanical Properties

An example of MA625 mechanical properties

Shape Tensile strength (kgf/mm2) 0.2%offse (kgf/mm2) Elongation (%) Hardness
Round(60φ) 95(≧84.4) 45(≧42.2) 56(≧30) HB192
Cold Roll(1.2t) 97(≧84.4) 50(≧42.2) 40(≧30) HRC 23 Hv 251
Hot roll(20t) 91(≧84.4) 44(≧42.2) 46(≧30) HRC21

Corrosion Resistance

Corrosion resistance of MA625